Impact Strength vs Temperture
Untitled Document

Public Reference(s): 1


Impact Strength (J)
Alloy -50ºC -20ºC 23ºC 75ºC 150ºC
AZ91 1.3 (0.2) 1.4 (0.1) 1.4 (0.1) 1.4 (0.2) 1.5 (0.1)
AM20 4.4 (0.2) 4.2 (0.4) 4.4 (0.2) 5.2 (0.2) 5.9 (0.5)
AM50 3.3 (0.2) 3.3 (0.3) 3.3 (0.4) 3.5 (0.1) 3.7 (0.5)
AM60 3.2 (0.2) 3.0 (0.1) 3.1 (0.2) 3.5 (0.2) 3.5 (0.4)
AE42 2.4 (0.2) 2.5 (0.2) 2.7 (0.1) 2.7 (0.4) 3.2 (0.4)
AS21 2.6 (0.1) 2.8 (0.2) 2.8 (0.2) 2.9 (0.2) 3.2 (0.3)
AS41 2.6 (0.2) 2.5 (0.1) 2.6 (0.2) 2.8 (0.4) 3.0 (0.1)

Standard deviation values in brackets.