Compression Strength

There is a significant difference at the 0.05 level (95% confidence) between all alloys, for all temperatures included, except between the alloys AS21 and AE42 at 25°C, 75°C and 175°C.


There is a significant difference at the 0.05 level (95% confidence) between all alloys, for all temperatures included, except between the alloys:

  • AS21 and AE42 at 25°C, 75°C, 125°C and 150°C
  • AM50 and AS21 at 25°C
  • AM50 and AE42 at 25°C and 75°C

Mean Compression Strength Values at Room Temperature
  AZ91 AM50 AM20 AS21 AE42
UTS (MPa) CVS (0.2% offset) 148 (3) 113 (4) 74 (2) 106 (1) 103 (4)
Compression Strength at 1% 182 (3) 138 (3) 93 (2) 134 (2) 137 (3)

Standard deviation values in brackets.


Test Information:

All these data are based on separately die cast test bars produced in a 40 ton cold chamber machine.

International Magnesium Association
1000 Westgate Drive, Suite 252  |  Saint Paul, Minnesota 55114 USA
P: +1 651.379.7305  |  F: +1 651.290.2266  |  E: info@intlmag.org