Tensile Testing, Effect of Strain Rate

Public Reference(s): 1





Alloy
Property
Crosshead Speed (mm/min)
0.5 1 20 100 200
AZ91 UTS (MPa) 246 (10) 243 (11) 250 (12) 246 (5) 252 (7)
TYS (MPa) 150 (5) 147 (7) 155 (6) 176 (5) 163 (23)
Elong. (%) 6.8 (1.0) 6.6 (0.8) 7.1 (1.2) 6.6 (0.6) 7.1 (0.9)
AM60 UTS (MPa) 246 (11) 250 (8) 253 (2) 246 (3) 247 (11)
TYS (MPa) 119 (5) 120 (3) 133 (7) 143 (4) 142 (3)
Elong. (%) 15.8 (2.2) 17.2 (2.5) 16.1 (1.8) 14.4 (1.7) 13.1 (2.7)

Standard deviation values in brackets.